10.2.1. Experimental Data

Experimental data for shear viscosity vs. shear rate are as follows:

  • visco_200.crv (viscosity vs. shear rate at 200° C):

     1.0476158e-01 4.7409219e+04
     1.2618569e-01 4.6221703e+04
     1.5199111e-01 4.4989727e+04
     1.8307383e-01 4.3684172e+04
     2.2051308e-01 4.2269406e+04
     2.6560879e-01 4.0711258e+04
     3.1992671e-01 3.8987227e+04
     3.8535285e-01 3.7095207e+04
     4.6415886e-01 3.5058137e+04
     5.5908102e-01 3.2921125e+04
     6.7341506e-01 3.0742695e+04
     8.1113082e-01 2.8582736e+04
     9.7700995e-01 2.6492119e+04
     1.1768119e+00 2.4505934e+04
     1.4174742e+00 2.2641396e+04
     1.7073526e+00 2.0899119e+04
     2.0565124e+00 1.9267033e+04
     2.4770765e+00 1.7725678e+04
     2.9836473e+00 1.6254397e+04
     3.5938139e+00 1.4836971e+04
     4.3287611e+00 1.3465704e+04
     5.2140083e+00 1.2142567e+04
     6.2802911e+00 1.0877272e+04
     7.5646334e+00 9.6834766e+03
     9.1116276e+00 8.5747520e+03
     1.0974989e+01 7.5614922e+03
     1.3219412e+01 6.6494995e+03
     1.5922827e+01 5.8398315e+03
     1.9179104e+01 5.1295151e+03
     2.3101297e+01 4.5126445e+03
     2.7825592e+01 3.9814446e+03
     3.3516029e+01 3.5272209e+03
     4.0370174e+01 3.1410603e+03
     4.8626015e+01 2.8143108e+03
     5.8570202e+01 2.5388992e+03
     7.0548027e+01 2.3074878e+03
     8.4975342e+01 2.1135415e+03
     1.0235312e+02 1.9513297e+03 
    
  • visco_220.crv (viscosity vs. shear rate at 220° C):

     1.0476158e-01 3.2600383e+04
     1.2618569e-01 3.1866336e+04
     1.5199111e-01 3.1115115e+04
     1.8307383e-01 3.0347666e+04
     2.2051308e-01 2.9555596e+04
     2.6560879e-01 2.8722006e+04
     3.1992671e-01 2.7824447e+04
     3.8535285e-01 2.6839762e+04
     4.6415886e-01 2.5750273e+04
     5.5908102e-01 2.4550127e+04
     6.7341506e-01 2.3249219e+04
     8.1113082e-01 2.1873061e+04
     9.7700995e-01 2.0457902e+04
     1.1768119e+00 1.9043281e+04
     1.4174742e+00 1.7664730e+04
     1.7073526e+00 1.6348507e+04
     2.0565124e+00 1.5109322e+04
     2.4770765e+00 1.3950688e+04
     2.9836473e+00 1.2866907e+04
     3.5938139e+00 1.1846350e+04
     4.3287611e+00 1.0875361e+04
     5.2140083e+00 9.9421738e+03
     6.2802911e+00 9.0399053e+03
     7.5646334e+00 8.1679702e+03
     9.1116276e+00 7.3314004e+03
     1.0974989e+01 6.5386035e+03
     1.3219412e+01 5.7986880e+03
     1.5922827e+01 5.1192021e+03
     1.9179104e+01 4.5048770e+03
     2.3101297e+01 3.9573066e+03
     2.7825592e+01 3.4752805e+03
     3.3516029e+01 3.0554553e+03
     4.0370174e+01 2.6930635e+03
     4.8626015e+01 2.3825698e+03
     5.8570202e+01 2.1181692e+03
     7.0548027e+01 1.8941488e+03
     8.4975342e+01 1.7051194e+03
     1.0235312e+02 1.5461493e+03 
    
  • visco_240.crv (viscosity vs. shear rate at 240° C):

     1.0476158e-01 2.2935412e+04
     1.2618569e-01 2.2492188e+04
     1.5199111e-01 2.2018766e+04
     1.8307383e-01 2.1526125e+04
     2.2051308e-01 2.1021365e+04
     2.6560879e-01 2.0505982e+04
     3.1992671e-01 1.9975033e+04
     3.8535285e-01 1.9417773e+04
     4.6415886e-01 1.8819420e+04
     5.5908102e-01 1.8164182e+04
     6.7341506e-01 1.7439488e+04
     8.1113082e-01 1.6640199e+04
     9.7700995e-01 1.5771608e+04
     1.1768119e+00 1.4849731e+04
     1.4174742e+00 1.3898310e+04
     1.7073526e+00 1.2944033e+04
     2.0565124e+00 1.2011361e+04
     2.4770765e+00 1.1118893e+04
     2.9836473e+00 1.0277535e+04
     3.5938139e+00 9.4904971e+03
     4.3287611e+00 8.7546172e+03
     5.2140083e+00 8.0624219e+03
     6.2802911e+00 7.4047461e+03
     7.5646334e+00 6.7733594e+03
     9.1116276e+00 6.1631475e+03
     1.0974989e+01 5.5731948e+03
     1.3219412e+01 5.0064775e+03
     1.5922827e+01 4.4684849e+03
     1.9179104e+01 3.9653857e+03
     2.3101297e+01 3.5024512e+03
     2.7825592e+01 3.0831277e+03
     3.3516029e+01 2.7087434e+03
     4.0370174e+01 2.3787000e+03
     4.8626015e+01 2.0908918e+03
     5.8570202e+01 1.8422029e+03
     7.0548027e+01 1.6289486e+03
     8.4975342e+01 1.4472250e+03
     1.0235312e+02 1.2931675e+03 
    

Experimental data for the storage and loss moduli ( and ) are as follows:

  • gprime.crv ( vs. angular frequency curve at 220° C):

     1.0000000e-01 5.9316000e+02
     1.5850000e-01 1.1784000e+03
     2.5120000e-01 2.2076000e+03
     3.9810000e-01 3.9173000e+03
     6.3100000e-01 6.5593000e+03
     1.0000000e+00 1.0419000e+04
     1.5850000e+00 1.5724000e+04
     2.5120000e+00 2.2596000e+04
     3.9813000e+00 3.1232000e+04
     6.3101000e+00 4.1570000e+04
     1.0001000e+01 5.3470000e+04
     1.5850000e+01 6.6881000e+04
     2.5121000e+01 8.1509000e+04
     3.9813000e+01 9.7119000e+04
     6.3101000e+01 1.1352000e+05
     1.0000000e+02 1.3036000e+05 
    
  • gsecond.crv ( vs. angular frequency curve at 220° C):

     to be replaced by :
     1.0000000e-01 3.2158000e+03
     1.5850000e-01 4.7820000e+03
     2.5120000e-01 6.9325000e+03
     3.9810000e-01 9.7403000e+03
     6.3100000e-01 1.3239000e+04
     1.0000000e+00 1.7346000e+04
     1.5850000e+00 2.2001000e+04
     2.5120000e+00 2.7050000e+04
     3.9813000e+00 3.2279000e+04
     6.3101000e+00 3.7352000e+04
     1.0001000e+01 4.2321000e+04
     1.5850000e+01 4.6851000e+04
     2.5121000e+01 5.1123000e+04
     3.9813000e+01 5.5108000e+04
     6.3101000e+01 5.9097000e+04
     1.0000000e+02 6.3270000e+04 
    

The files for these data curves are provided on the Ansys Polyflow product CD, in the test/polymat/example2 subdirectory.